ABS Characteristics: High hardness, good gloss, moderate flowability, susceptibility to moisture absorption, tendency to develop internal stress, poor heat resistance, susceptibility to scorching, and proneness to cracking. It is the most commonly used material for home appliances, daily necessities, and electronic enclosures.
I. Silver Streaks / Water Marks / Air Voids
Phenomenon: Silver-white thread-like patterns, a misty appearance, or water-mark-like streaks on the surface.
Causes:
- Raw material contains moisture and has not been dried.
- Material temperature is excessively high, leading to decomposition and gas generation.
- Injection speed is too fast, causing air entrapment.
- Poor venting in the mold.
- Insufficient back pressure, resulting in poor plasticization and venting.
Solutions:
- Dry the material at 80–85°C for 2–3 hours (drying is mandatory).
- Appropriately lower the barrel temperature.
- Reduce the injection speed during the initial phase to prevent air entrapment.
- Improve mold venting channels to eliminate trapped air.
- Increase back pressure to ensure more uniform plasticization.
II. Cracking / Stress Cracking / Boss Bursting
Symptoms: Cracking during demolding, cracking during assembly, cracking after storage, boss fracture
Causes:
- Excessive internal stress (high injection speed, high shear stress, low mold temperature)
- Mold temperature too low; cooling rate too rapid
- Uneven ejection; ejector marks (whitening)
- Insufficient draft angle; surface tearing
- Cracking induced by contact with chemicals or oil contaminants
Solutions:
- Increase mold temperature to 50–70°C
- Reduce injection speed; minimize shear stress
- Adjust ejector pin layout; increase ejection area
- Increase the draft angle
- Avoid contact with organic solvents; anneal if necessary
III. Short Shots / Insufficient Flow / Incomplete Filling
Symptoms: Unfilled sharp corners, thin-walled sections, deep ribs, and distal areas.
Causes:
- Material temperature / Mold temperature is too low.
- Injection pressure and injection speed are insufficient.
- Runners / Gates are too small.
- Poor venting; trapped air obstructs material flow.
- Back pressure is insufficient, resulting in uneven plasticization.
Solutions:
- Increase material temperature to 200–240°C.
- Increase injection pressure and injection speed.
- Enlarge the gates and runners.
- Improve venting.
- Increase back pressure to ensure proper plasticization.
IV. Prominent Weld Lines and Poor Strength
Phenomenon:The convergence line is deep, appears whitish, and forms a distinct visible line.
Causes:
- Material temperature and/or mold temperature are too low.
- Injection speed is too slow, causing the flow front of the material to cool prematurely.
- Poor venting leads to air entrapment at the convergence point.
- The gate location is inappropriate, resulting in an excessively long flow path.
Solutions:
- Increase the material temperature and mold temperature.
- Appropriately increase the injection speed.
- Add vents at the location of the weld line.
- Optimize the gate placement to shorten the flow path.
V. Bubbles / Voids
Phenomenon: Surface bubbles, internal voids
Causes:
- Raw material contains moisture, which vaporizes at high temperatures
- Melt temperature is too high, causing decomposition and gas generation
- Injection speed is too fast, resulting in air entrapment
- Insufficient holding pressure; material not fully compacted
- Shrinkage in thick-walled sections creates vacuum voids
Solutions:
- Thoroughly dry the raw material
- Lower the melt temperature
- Use a slower injection speed to fill the mold and minimize air entrapment
- Increase holding pressure and extend the holding time
- For thick-walled parts, extend both the holding time and the cooling time
VI. Flash / Burrs
Symptom: Material overflow at the parting line, inserts, or ejector pin locations.
Causes:
- Material temperature is too high.
- Injection pressure / speed is excessive.
- Clamping force is insufficient.
- Excessive clearance in mold mating surfaces.
- Injection volume is excessive (overfilling).
Solutions:
- Lower the material temperature.
- Reduce injection pressure and speed.
- Increase clamping force.
- Modify the mold to reduce clearance.
- Reduce the metering volume to avoid overfilling.
VII. Scorching, Black Spots, Black Streaks, and Yellowing
Phenomena:Black spots, scorched patches, yellowing, burnt corners/edges.
Causes:
- Material temperature is excessively high; ABS undergoes thermal decomposition.
- Material dwell time within the screw is too long.
- Poor venting leads to trapped air and high temperatures caused by compression.
- Carbon buildup within the barrel results in black spots.
- Injection speed is too fast, causing excessive shear heating.
Solutions:
- Lower the material temperature and shorten the cycle time.
- Purge the barrel completely before shutting down the machine.
- Improve venting to prevent air entrapment.
- Clean the barrel and the screw.
- Reduce the injection speed to minimize shear heating.
VIII. Shrinkage / Sink Marks
Phenomenon: Sink marks on thick-walled sections, ribs, and the backs of bosses.
Causes:
- Insufficient holding pressure; short holding time.
- Injection pressure is too low.
- Gate is too small, leading to premature freezing.
- Melt temperature and/or mold temperature are too high.
- Uneven wall thickness.
Solutions:
- Increase holding pressure; extend holding time.
- Appropriately increase injection pressure.
- Enlarge the gate; delay gate freezing.
- Appropriately lower the melt temperature and mold temperature.
- Design the product with as uniform a wall thickness as possible.
IX. Warpage and Deformation
Phenomena: Bending, twisting, dimensional instability
Causes:
- Uneven cooling; high internal stress
- Mold temperature too low, or significant temperature difference between the front and rear mold halves
- Uneven wall thickness; inconsistent shrinkage
- Excessively high injection speed; severe molecular orientation
- Unbalanced ejection
Solutions:
- Increase and equalize mold temperature; extend cooling time
- Reduce injection speed to minimize molecular orientation
- Optimize wall thickness design
- Adjust ejection balance
- Perform annealing treatment if necessary
X. Ejector Whitening, Protrusion, and Cracking
Phenomena: Whitening, protrusion, or cracking at the ejector pin locations.
Causes:
- Low mold temperature, resulting in a brittle part.
- Unbalanced ejection; undersized ejector pins.
- Ejection initiated before sufficient cooling has occurred.
- Insufficient draft angle; high mold-clamping force (part adhesion).
- High internal stress within the part.
Solutions:
- Increase the mold temperature.
- Use larger-diameter ejector pins or increase the number of pins.
- Extend the cooling time.
- Increase the draft angle.
- Optimize processing parameters to reduce internal stress.
XI. Poor Gloss, Matte Finish, Dull Surface
Phenomenon: Surface lacks luster, appears hazy or rough/pitted.
Causes:
- Mold temperature is too low.
- Material temperature is insufficient.
- Mold surface is rough.
- Poor venting.
- Raw material contains moisture.
Solutions:
- Increase mold temperature to 50–70°C.
- Appropriately increase material temperature.
- Polish the mold surface.
- Improve venting.
- Ensure raw material is dry.